Use only those adhesives which are suitable for joining PVC
products.
After applying the adhesive, wait at least 24 hours before con-
ducting a pressure test.
7.2.2.
heating element socket welding
(pp-h, pVdF)
Procedure:
Chamfer the pipe ends by approx. 15°.
Check outer diameter of pipe / inner diameter of the socket
according to the following table.
nominal width
pipe
dn
outer Ø
[mm]
[mm]
10
16
15
20
20
25
25
32
32
40
40
50
50
63
16
socket
inner Ø
[mm]
15.85 ... 15.95
19.85 ... 19.95
24.85 ... 24.95
31.85 ... 31.95
39.75 ... 39.95
49.75 ... 49.95
62.65 ... 62.95
english
Type 2657
Installation
Set the temperature controller of the welding equipment to
250 - 270 °C.
Observe the warming-up time, welding time and cooling- down
time according to the following tables.
Leave the welded joints to cool down always at room
temperature!
Welding parameters
nominal
pipe
Minimum thickness
width
outer
[mm]
dn
Ø
[mm]
[mm]
10
16
2.5 (PP-H) - 1.5 (PV DF)
15
20
2.5 (PP-H) - 1.9 (PV DF)
20
25
2.7 (PP-H) - 1.9 (PV DF)
25
32
3.0 (PP-H) - 2.4 (PV DF) 8 (PP-H) - 10 (PV DF)
32
40
3.7 (PP-H) - 2.4 (PV DF) 12 (PP-H) - 12 (PV DF)
40
50
4.6 (PP-H) - 3.0 (PV DF) 16 (PP-H) - 18 (PV DF)
50
63
3.6 (PP-H) - 3.0 (PV DF) 24 (PP-H) - 20 (PV DF)
Warming up time
[s]
5 (PP-H) - 4 (PV DF)
5 (PP-H) - 4 (PV DF)
7 (PP-H) - 8 (PV DF)

Publicité