STAMOS S-MIG 250C Manuel D'utilisation page 23

Table des Matières

Publicité

Les langues disponibles
  • FR

Les langues disponibles

  • FRANÇAIS, page 37
EN
Disturbance
Cause & solution
Oxidized appearance
Apply a long arc in the
groove
of welds
Adjust voltage
Wire bent or extending
too far from the wire
guide
Incorrect wire feed
speed
Insufficient penetration
Irregular or inadequate
of the root
spacing
Incorrect angle of the
welding torch
Wire guide tube worn
Wire feed speed is too
low for the voltage or
the welding speed
Penetration
Wire feed speed too
high
Incorrect angle of the
welding torch
Spacing too large
44
Example
EN
Rapid Search Table
I-shaped Butt Welding
Plate thick-
Gap g(mm)
Solder wire
Welding
ness t(mm)
diameter
current (A)
(mm)
0,8
0
0,8 - 0,9
60 - 70
1,0
0
0,8 - 0,9
75 - 85
1,2
0
1,0
70 - 80
1,6
0
1,0
80 - 100
2,0
0 - 0,5
1,0
100 - 110
2,3
0,5 - 1,0
1,0 / 1,2
110 - 130
3,2
1,0 - 1,2
1,0 / 1,2
130 - 150
4,5
1,2 - 1,5
1,2
150 - 170
Fillet Weld Seam in flat position
45
Welding
Welding
Gas flow (L/
voltage (V)
Speed (cm/
Min)
Min.)
16 - 16,5
50 - 60
10
17 - 17,5
50 - 60
10 - 15
17 - 18
45 - 55
10
18 - 19
45 - 55
10 - 15
19 - 20
40 - 55
10 - 15
19 - 20
50 - 55
10 - 15
19 - 21
40 - 50
10 - 15
21 - 23
40 - 50
10 - 15