It is recommended to make some preliminary welding tests if other consumables are used.
Thickness of the support sheet metal (value
To increase or decrease the sheet metal thickness to which the insert will be welded use keys D+ and D-.
If the thickness of the sheet metal is less than that shown on the display, a marking on the rear of the weld may appear.
When the station displays «
an optimal weld.
If this pictogram does not appear, then the maximum sheet metal thickness has been reached. Beyond this thickness,
the welding of the insert is no longer guaranteed.
Power coefficient (value
The Power coefficient is used to adjust the ignition current, the arc energy (current, time) and the attachment current.
Power can be adjusted between -10 and +10. To increase or decrease this coefficient press keys G+ and G-.
Note: Weld synergies are optimized with a default Power coefficient value of 0.
Power
Action on the product
• Increase the ignition current
• 2% increase in arc current up to 200A, then
+1 point
3% increase in arc time up to 500ms.
• Increase the attachment current.
• Decrease the ignition current
-1point
• 2% reduction of the arc current.
• Decrease of the attachment current."
To change the other synergistic welding parameters (materials, type and size of insert, gas) refer to the chapter «Syner-
gistic Settings».
WELDING IN MANUAL MODE
In Manual Mode, times,currents, coefficients for the different welding phases and the lifting height of the insert need
to be set by the user.
Ring
Fe
+1
To increase or decrease the arc duration (value
To increase or decrease the arc current (value
To change the other synergistic welding parameters (materials, type and size of insert, gas) refer to the chapter «Manual
OVERVOLTAGE DEFECT
Settings».
COM. DEFECT
24
SPOT ARCPULL 200
Type, material and size of
insert
Coefficient Power
», the sheet thickness is high enough so that it is not marked on the back while having
)
1.5mm
Gas
2.0
Arc duration
zone de
message
message
area
t
ms
100
zone de
message
Goujon
M5
Fe
ArCO_8%
+1
3.0
zone de
message
)
Influence on the weld
• Better arc ignition on poorly degreased sheet
metal..
• Better ignition in cold weather (<5°C).
• 2% increase of arc energy.
• Reduced risk of sticking during ignition.
• Suitable ignition in hot weather (>35°C).
• 2% decrease of arc energy.
t
I
ms
A
100
200
message
area
t
I
ms
A
), use the keys G+ and G-.
100
100
I
A
), use the keys D+ and D-.
100
zone de
OVERHEATING DEFECT
message
PRESSED KEY
Gas to use
Sheet metal thickness
Main Menu
> Settings
Manual Mode
Configuration
Arc current
Configuration
> Pregas
> 100ms
Postgas
500ms
Language
EN
Product reset
Info
Manual Settings
Start-up
> Q = 0
Synergic Settings
EN

Publicité

loading